Uniaxial Tension (Room Temperature)
Uniaxial tensile tests are performed to GB/T 228-2002, GB/T 5027-1999 and GB/T 5028-1999 in order to obtain material property data for sheet metals.
Specimen Size
Three orientations (0°, 45° and 90° to the rolling direction°) specimens undergo uniaxial tensile tests with three repeats per item; blanks are machined to GB/T 228-2002 dimensions.

Uniaxial Tensile Specimen Dimensions
Tests are performed on an electronic universal testing machine, as shown.

Electronic Universal Testing Machine
Uniaxial tensile data are processed by averaging the two most repeatable runs out of three for each item.
Mechanical properties of a material are listed below:

True stress–true strain curve as shown:

Uniaxial Tension (High Temperature)
Hot uniaxial tensile tests are performed on an electronic high-temperature universal testing machine (200–1000 °C). The furnace uses resistance radiation heating with three thermocouples controlling top, middle and bottom zones to ±3 °C. Specimens are held at temperature for 5 min to ensure uniform deformation. Constant-strain-rate tension is achieved by speed-controlled software; specimens cool to room temperature in the furnace afterwards. Tests at various temperatures and strain rates are possible.


Hot uniaxial tensile test conditions for a titanium alloy are as follows:

The hot titanium alloy is treated as isotropic; specimens at 0° to the extrusion direction are studied, as shown:

The machine records engineering stress–strain, which is converted to true stress–strain as shown.



Uniaxial Tension (Low Temperature)
With a liquid-nitrogen temperature chamber (−70 °C to 200 °C), low-temperature uniaxial tensile tests are possible.